PCB processes


Panelization is a procedure whereby a number of PCBs are grouped for manufacturing onto a larger board - the panel. Usually a panel consists of a single design but sometimes multiple designs are mixed on a single panel. There are two types of panels: assembly panels - often called arrays - and bare board manufacturing panels. The assembler often mount components on panels rather than single PCBs because this is efficient. The bare board manufactures always uses panels, not only for efficiency, but because of the requirements the plating process. Thus a manufacturing panel can consist of a grouping of individual PCBs or of arrays, depending on what must be delivered.

Chemical etching is usually done with ammonium persulfate or ferric chloride. For PTH (plated-through holes), additional steps of electroless deposition are done after the holes are drilled, then copper is electroplated to build up the thickness, the boards are screened, and plated with tin/lead. The tin/lead becomes the resist leaving the bare copper to be etched away.

The simplest method, used for small-scale production and often by hobbyists, is immersion etching, in which the board is submerged in etching solution such as ferric chloride. Compared with methods used for mass production, the etching time is long. Heat and agitation can be applied to the bath to speed the etching rate. In bubble etching, air is passed through the etchant bath to agitate the solution and speed up etching. Splash etching uses a motor-driven paddle to splash boards with etchant; the process has become commercially obsolete since it is not as fast as spray etching. In spray etching, the etchant solution is distributed over the boards by nozzles, and recirculated by pumps. Adjustment of the nozzle pattern, flow rate, temperature, and etchant composition gives predictable control of etching rates and high production rates.

As more copper is consumed from the boards, the etchant becomes saturated and less effective; different etchants have different capacities for copper, with some as high as 150 grams of copper per litre of solution. In commercial use, etchants can be regenerated to restore their activity, and the dissolved copper recovered and sold. Small-scale etching requires attention to disposal of used etchant, which is corrosive and toxic due to its metal content.

The etchant removes copper on all surfaces exposed by the resist. "Undercut" occurs when etchant attacks the thin edge of copper under the resist; this can reduce conductor widths and cause open-circuits. Careful control of etch time is required to prevent undercut. Where metallic plating is used as a resist, it can "overhang" which can cause short-circuits between adjacent traces when closely spaced. Overhang can be removed by wire-brushing the board after etching.

If you need expert PCB services, please feel free to contact me, wonderful02@wonderfulpcb.com

2015年3月13日星期五

Why use surface mount technology (SMT)?

Currently, advanced electronic products, especially in the computer and communications electronics products, has been widely used in SMT technology. SMD devices on year rise in international production, but production is declining conventional device, so as time goes into between, SMT technology will become increasingly popular.
So what is the advantage of SMT in circuit board manufacturing?
1,The pursuit of the miniaturization of electronic products, perforated and plug components used previously been unable to narrow.

2, The electronic product features become more complete, integrated circuit (IC) is no longer used by the piercing element, especially in large-scale, highly integrated IC, had to use surface mount components.

3, Bulk products, production automation, factory should take a low-cost high-volume, producing high quality products to meet customer demand and enhance market competitiveness

4, The development of electronic components, integrated circuits (IC) development, multi-application of semiconductor materials

5, Electronic technology revolution is imperative, chasing the international trend

SMT has become a mainstream technology in the era of high-density, due to the use of SMT technology, PCBA  also follow up and get rapid development. SMT market share surge makes more stringent, good PCBA SMT is a prerequisite for success. SMT mainly from the process to control the quality of the process. Today we will introduce single Sided SMT assembly process.

Single Sided SMT assembly process:

Incoming inspection -> screen printing solder paste (dot patch glue) -> patch -> drying (curing) -> reflow soldering -> Cleaning -> Test -> Rework

2015年3月11日星期三

CES 2015: The future of wearable technology

Flexible PCB board devices for clothing, virtual-reality contact lenses and tools to help hearing impediments are some of the futuristic use cases for rapidly emerging wearables.

"We should not be trying to make tech wearable, but rather make wearable things technology-enabled," according to Mike Bell, the vice president and general manager of Intel’s new devices group.
Speaking in Las Vegas today on a CES 2015 panel about the growth of wearables, Bell discussed the challenges manufacturers and brands in the space must overcome to break into the mainstream.
He said a "cellphone on the wrist" [the smartwatch has become the poster child for wearables] is not what people want, and wearable tech will start moving into items like jewellery and watches.
Wearable tech gets its share of bad press for a wide range of reasons, including its failure to look good and demonstrate utility for consumers. Reports have shown that current devices, such as fitness trackers, are often abandoned several months after use.
Despite the challenges the category faces, the panellists were bullish on wearable tech’s future, confident the devices are not a technology fad.
Christopher Glode, the general manager at Under Armour Connected Fitness, said: "The market valuation of wearables is not really relative to the amount of hype they get, but real markets are being created around wearables now.
"Sensors are getting smaller, batteries are lasting longer and the technology is evolving very, very quickly, piggybacking on smartphones, which means more things are possible now."
Bell added that wearable devices are more accepted these days because of the rise of smartphones, legitimising the need for consumers to have a device with them all the time.
But wearables will not replace smartphones any time soon, the panel argued.
"The phone will become even more important as a hub for experience," Glode said.
Carmichael Roberts, a partner at North Bridge, the venture capitalists, said that wearable tech would continue to innovate in the direction of something "invisible, seamless, comfortable and very personal," blurring the boundary between humans and computers.
"People won’t think about it, like they don’t think about having tattoos on their skin, like a stamp or a sticker," he said.
Limor Schafman, the founder and chief executive of GlobeShift, said the major future developments in the wearables space would be in flexible wearables that can become part of clothing, contact lenses with virtual reality and technology to help people with hearing impairments.
"There is no limit to the imagination of what is possible," Schafman said. "What is fascinating is that the technology is here. Now, what do we do with it?"
This story has been taken from Campaign US.
This article was first published on campaignlive.co.uk

2015年3月5日星期四

Immersion tin

For nowadays all the solder material is tin-based, the tin layer can be matched with any type of solder, In this point, immersion tin process is very promising. However years ago, Aluminum pcb will exits tin whiskers after immersion tin process and tin migration and tin whiskers shall bring reliability problems in the welding which limited the use of immersion tin process. Later we found the solution that adding tin organic additives to the immersion tin liquid which makes tin layer to become granular structure, well solved the problems, and also make better thermal stability and weldability.
Immersion tin process can form the flat copper-tin intermetallic compounds, this feature makes the immersion tin has the same good weldability as hot air leveling but without the headaches flatness problem; Also do not have proliferation issues between gold metal compared to Electroless Nickel / Immersion;
But the immersion tin plate can not be stored for a long time.

2015年3月4日星期三

Aluminum board process-B

5.4 Aluminum pcb inspection
5.4.1 line surface must be in accordance with the requirements of the MI to check all the content.
5.4.2 must check on aluminum surface, aluminum surface dry film cannot have film falls and broken.
5.5 etching
5.5.1 for copper base is commonly 4 oz, will there is a certain difficulty in etching.First plate must be approved by the captain in person to do board, made in the spot check, line width, line spacing should be strengthened once every 10 PNL plate spot check line width, and make records.
5.5.2 recommended parameters: speed: 7 ~ 11 dm/min pressure: 2.5 kg/cm2 proportion: 25 be temperature: 55 ℃ (the above parameters are for reference only, the test plate results shall prevail)
5.5.3 back membrane should be paid attention to the time of the control between 4 ~ 6 min, because aluminium will reaction with NaOH, but also must ensure that the membrane clean, backing down membrane liquid membrane was not allowed to turn up the heat.No protective film of the plate, aluminum, from liquid membrane in the back up after the board will not stay to wash water on a board in time of liquid membrane, prevent the alkali corrosion of aluminum surface.  
5.6 corrosion inspection
5.6.1 normal board.
5.6.2 it is forbidden to use the blade repair line, in order to avoid injury and dielectric layer.
5.7 the solder mask
5.7.1 production process:
Brush copper surface grinding plate (only) to screen printing green oil (the first), and preliminary drying screen printing green oil (second) and the preliminary drying - exposure and development - plate mill, the acid pickling process. Under the soft brush - after curing -
5.7.2 reference parameters:
5.7.2.1 yarn used 36 t + 100 t
First 75 ℃ 5.7.2.2 x 20-30 min;The second 75 ℃ x 20-30 min
5.7.2.3 exposure: 60/65 (single) 9 ~ 11
5.7.2.4 enhancement: speed: 1.6 ~ 1.8 m/min pressure: 3.0 kg/m2 (total pressure)
5.7.2.5 curing: after 90 ℃ * 60 min + 60 min + 110 ℃ 150 ℃ above x 60 min parameters for the use of the DSR - 2200 tl ink, used only for reference.
5.7.3 note printing for control of air bubbles, if need, can add 1-2% of the diluent.
5.7.4 clappers before clappers member should check panel, there is a problem of instruct the captain and then to the clapper.   
5.8 HASL
5.8.1 spray before tin for aluminum plate with protective film tear protective film after spray tin.    
5.8.2 edge with both hands, it is strictly prohibited by hand directly touch the plate (especially aluminum surface).
5.8.3 operation, fight chafed.
5.8.4 tin cookie sheet before 130 ℃, 1 hour, and baking sheet to spray tin interval time less than 10 minutes.In order to avoid temperature difference cause a layered with ink.    
5.8.5 rework plate spray is only allowed to return once, if more than one board, to distinguish for special treatment.    
5.9 aluminum surface passivation treatment
5.9.1 level passivation process: (1) scrubbing brush (500 #) to (2) water - > (3) passivation, (4) washing the x 3-5. Dry - 6 drying
Note: (1) grinding plate: only aluminum surface grinding, FR4 parameter grinding plate.First board to check line no scratches, as well as the tin cried, uniform grinding crack.
(3)passivation: potion ingredients open cylinder quantity cylinder volume liquid temperature control concentration spraying in tank pressurization rate
Na2CO3 (CP) 50 g / 6500 g l, 130 l, 40 ~ 50 ℃ 2.0 ~ 3.0 1.0 ~ 1.5 m/min effective soaking time 10 ~ 15 s 100 m2 CP (K2CrO4) 15 g/l,  1950 g NaOH (CP) 390 g, 3 g/l
6 drying: 80 ~ 90 ℃.
Tyle = "the oledata.mso - spacerun: 'yes', the font size: 10.5000 pt; the font-family:" tahoma "; "> 5.7.2.5 curing: after 90 ℃ * 60 min + 60 min + 110 ℃ 150 ℃ above x 60 min parameters for the use of the DSR - 2200 tl ink, used only for reference.
5.7.3 note printing for control of air bubbles, if need, can add 1-2% of the diluent.   
5.7.4 clappers before clappers member should check panel, there is a problem of instruct the captain and then to the clapper.  

2015年3月3日星期二

System Level Design for My Bluetooth LED Lamp

System Level Design for My Bluetooth LED Lamp, yes I make Visio drawings for fun.
You may not know specifics like what supply voltages you will need or what connections need to be made, but you will be able to consider how each component will rely on the others and what additional components they will add to your design.
This is also a good time to consider the aesthetic aspect of your design. Are you trying to fit a certain form factor? Do you need to consider ergonomics (for example if you are designing a game controller)? Will you be able to pick up your design a year from now and understand exactly how it works? These are the types of details Aluminum pcb, while seemingly insignificant, can be the difference between a good design and a great design.
I know all this talk of visualization may sound cheesy and like it won’t really get you anywhere, but I assure you it is worthwhile. If you don’t want to believe me, consider this quote from Nikola Tesla’s autobiography where he describes his creative process:
My method is different. I do not rush into actual work. When I get an idea I start at once building it up in my imagination. I change the construction, make improvements and operate the device in my mind. It is absolutely immaterial to me whether I run my turbine in thought or test it in my shop. I even note if it is out of balance. There is no difference whatever, the results are the same.
Of course the vast majority of us aren’t at the level of crazed genius that is Tesla, but the idea behind this method is all the same. By visualizing your design beforehand you save time, money, and frustration.
Following will be continued in next chapter.
Shirley Xia
Wonderful PCB
T +86-755-86229518-636
e  wonderful25@wonderfulpcb.com |